Ewe, ukuwelda nge-17-4 PH kuyinto eqhelekileyo, kwaye umgangatho awudingi kufudunyezwa kwangaphambili ngendlela i-410 okanye i-420 efunekayo ngayo. Into efunekayo kukugcwalisa okufanelekileyo kunye nonyango lobushushu emva kokuwelda, kwaye unyango lugqiba ngakumbi malunga nejoyinti egqityiweyo kunokuba igcwalisa.

URui ujongene nokuwelda kumvelisi wepompo ngaphandle kwePorto. Ngowama-2023 ivenkile yakhe yakha ibracket yokufaka ye-17-4 PH ene-ER630 filler, yasebenzisa i-radiograph ecocekileyo, yaza yathunyelwa. Emva kweenyanga ezilishumi elinesine ibracket yaqhekeka, kungekhona kwi-weld kodwa kwi-band encinci yesinyithi esisezantsi ecaleni kwayo.

Isihluzi besichanekile. Inkqubo yayingenjalo, kuba akukho nto yenziweyo kwindawo echaphazelekileyo bubushushu emva kokuba i-arc icimile.

Mhlawumbi uxelelwe ukuba usebenzise i-ER630 kunye ne-heat treat. Elo cebiso lichanekile, kwaye luluhlu lokuqala lwenkqubo endaweni yokuba lonke libe linye. Eli nqaku ligubungela izigqibo ezine ezilawula i-17-4 PH weld: imeko, ukuzalisa, indlela emva kokuwelda kunye nokugqitywa. Likwagubungela nokuvuthuza kwe-arc, phantse akukho mntu ukulumkisayo ngayo.

Isikhokelo esipheleleyo sentsimbi engagqwaliyo ye-17-4 PH sigubungela umgangatho ngokwawo. Ukuba ubhala inkqubo yejoyinti yokwenyani, inkonzo yethu yokubonisana ngobuchwephesha iya kujonga imeko kunye nonyango lobushushu ngaphambi kokuba kudlule okokuqala.

IItrakthi ezibalulekileyo

  • Ukuwelda kwe-17-4 PH kufuna isizalisi esihambelanayo kunye nonyango lobushushu emva kokuwelda, kwaye unyango lugqiba ilungu. Isizalisi esichanekileyo esingenayo i-PWHT sinika ilungu elibi kunesizalisi se-austenitic esine-anneal epheleleyo yokucombulula.
  • I-ER630 kunye ne-E630 zezona zizalisi zihambelanayo phantsi kwe-AWS A5.9 kunye ne-A5.4. Isinyithi esitshisiweyo sigcwele i-martensitic kwaye asinayo i-delta ferrite, ngoko ke sinoqhekeko oluphezulu kwaye sifuna i-PWHT ukuze ifikelele kwiimpawu zayo.
  • Ukuwelda kwiMeko A. Ukuwelda inxalenye ye-H900 kuyayiphinda i-austenitize i-HAZ kwaye ishiye i-martensite engavuthwanga ecaleni kwe-weld, kwaye i-assembly ayisayi kuhambelana nesatifikethi sayo.
  • Kukho iindlela ezintathu ze-PWHT: isisombululo se-anneal kunye nobudala, ubudala kuphela, okanye akukho nto nge-austenitic filler. Kuphela yeyokuqala ebuyisela iipropati zesiseko-sentsimbi kuyo yonke ijoyinti.
  • Yipholise ngaphambi kokuba uyipholise. Ubushushu buyi-oxide ephelelwe yi-chromium, kwaye ukuyipholise phezu kwayo kuyayivala indawo yayo.

Yintoni i-17-4 PH Welding? Impendulo emfutshane

Yintoni i-17-4 PH Welding? Impendulo emfutshane
Yintoni i-17-4 PH Welding? Impendulo emfutshane

Ukuwelda kwe-17-4 PH kukudibanisa kwe-UNS S17400 yi-GTAW, GMAW, SMAW okanye i-SAW kunye nesihluzi se-ER630 esihambelanayo, kulandele unyango lobushushu emva kokuwelda. Udidi lunokuwelda kwiMeko A, kwaye amacandelo amancinci awadingi kufudumeza kwangaphambili. Iimpawu ezipheleleyo zamalungu zifuna isisombululo kunye nokuguga, okanye ubuncinane ukudlula kokuguga.

inkqubo Ifomu yokugcwalisa Ukusetyenziswa okuqhelekileyo amaNqaku
I-GTAW (TIG) Ucingo olungenanto lwe-ER630 Iingcambu ziyadlula, iindawo ezincinci, amalungu abalulekileyo Ulawulo olungcono; ukuvuthuza kwe-arc kwi-DC
I-GMAW (MIG) Ucingo olungenanto lwe-ER630 Iifillets zemveliso kunye namacandelo atyebileyo Ukubekwa okuphezulu; umngcipheko ofanayo wokubetheka kwe-arc
I-SMAW (intonga) I-electrode egqunywe yi-E630 Umsebenzi wasentsimini, ukulungiswa, ukufikelela okungafikelelekiyo Imicimbi yokugcina i-hydrogen ephantsi
ISITO Intambo ye-ER630 kunye ne-flux Imithungo emide ethe tye, iindawo ezinzima Igalelo eliphezulu lobushushu; jonga ubulukhuni be-HAZ

Ngaba ke ngoko ungawelda i-17-4 PH? Ewe. Ukuwelda kwe-TIG ye-17-4 PH kunye nokuwelda kwe-MIG kusebenzisa izixhobo ezifanayo nakweyiphi na ivenkile engenazintsimbi esele isebenza, kwaye umgangatho ngumsebenzi oqhelekileyo kwi-aerospace, ulawulo lokuhamba kwamanzi kunye nokuveliswa kwepompo.

Ingaba i-17-4 PH iyaxhunyelwa ngengqiqo yokuba ibalulekile kwezorhwebo? Kwakhona ewe, kodwa isiqinisekiso yingongoma. Ijoyinti exutyiweyo eshiywe yodwa ayifani neyo ixunyekwe yaza yalungiswa. Isizalisi sigqiba ngentsimbi exutyiweyo. Unyango lobushushu lugqiba ngejoyinti.

Kutheni i-17-4 PH iWelda ngendlela eyahlukileyo kwi-304 kunye ne-316

Umahluko koko kwenzekayo xa kuphola. Amanqanaba e-Austenitic ahlala e-austenitic, kwaye ipesenti ezimbalwa ze-delta ferrite zishiywa ngabom kwi-weld ukuze zimelane nokuqhekeka kokuqina. I-17-4 PH iguquka ibe yi-martensite njengoko iphola, kungekho ferrite eya kuncitshiswa kwaye akukho austenite yokufunxa uxinzelelo.

Oko kuphelisa imikhwa emithathu eziswa ngumchweli we-304 okanye we-316. Ukubalwa kweFerrite akuthethi nto apha, ukufakelwa kobushushu obuphantsi kolawulo lokuzivala akusiwo umqobo wokubopha, kwaye "akukho nyango lufunekayo emva kokuwelda" akulunganga.

Umahluko omkhulu yimeko yokuqala. Ipleyiti ye-304 ifika kwimeko eza kusebenza kuyo. Ipleyiti ye-17-4 PH ifika isisombululo sitshixiwe okanye sigugile, kwaye i-arc iyayitshabalalisa loo nto kwibhendi ebanzi ngeemilimitha ezimbalwa. Yonke enye into ilandela emva koko.

Isikhokelo sethu sokuwelda se-304 vs 316 sigubungela icala le-austenitic, apho kungekho nanye kwezi zinto isebenzayo.

Isinyithi sokuzalisa se-17-4 PH Welding: ER630, Austenitic, okanye Nickel-Base

Kukho iimpendulo ezintathu kumbuzo wesinyithi we-17-4 PH filler, kwaye zitshintshana amandla xa zithelekiswa nexesha lesithando.

I-ER630 yintambo engenanto ehambelanayo phantsi kwe -AWS A5.9 , kwaye i-E630 yi-electrode egqunyiweyo phantsi kwe-AWS A5.4. Intsimbi yokuzalisa ye-ER630 ifaka malunga ne-17Cr-4Ni-4Cu-Nb, ehambelana ne-UNS S17400. Yiyo yodwa i-filler efikelela kumandla esiseko sesinyithi, kwaye ifuna i-PWHT ukuze ifike apho.

I-Austenitic ER308L okanye i-ER309L iqinile, ixolela kwaye ayifuni ziko. Ijoyinti iwela ngaphantsi kwamandla esiseko sesinyithi, kwaye i-HAZ iseseyi-martensitic, ngoko utshintshise ipropathi ephambili yenqanaba ukuze kube lula. Loo nto yindlela yokurhweba, hayi indlela emfutshane.

Isithambisi se-nickel seklasi ye-ERNiCr-3 senzelwe amalungu entsimbi yekhabhoni angama-17-4 PH kwaye kwiimeko apho ulawulo lokunyibilikisa okanye ukujikeleza kobushushu kuphambili.

I-17-4 PH vs 15-5 PH kukuthelekisa ukusebenza ngaphambi kokucacisa ii-weldments zecandelo elinzima, kuba i-15-5 PH ixolela ngakumbi kumsebenzi onzima.

I-Filler Metal ngohlobo oludibeneyo

Joint Filler PWHT Amandla adibeneyo okwenyani
17-4 PH ukuya kwi-17-4 PH, amandla abaluleke kakhulu ER630 kufunwa Isondela kwi-base metal emva kwesisombululo se-anneal kunye nobudala
17-4 PH ukuya kwi-17-4 PH, ayibalulekanga kangako I-ER308L okanye i-ER309L Ingashiywa Isinyithi esingaphantsi kwesiseko; i-HAZ isese-martensitic
17-4 PH ukuya kwi-304 okanye kwi-316 I-ER309L, okanye i-ER630 apho amandla alawula khona Ulandela isigqibo samandla Isetiwe ngokupheleleyo ngokukhetha isizalisi
17-4 PH ukuya kwintsimbi yekhabhoni I-ER309L okanye isiseko se-nickel Ubushushu bulandela intsimbi yekhabhoni Inqunyelwe yi-carbon steel HAZ
17-4 PH ukuya kwi-15-5 PH ER630 kufunwa Igubungela amanqanaba omabini

Ukuwelda intsimbi yekhabhoni eyi-17-4 PH yeyona nto ibamba abantu. Imithetho yokushisa nokudlulisa intsimbi ivela kwintsimbi yekhabhoni, hayi kwi-stainless, kwaye ukuxutywa kwi-martensitic deposit kubeka umngcipheko.

Kutheni i-ER630 Weld Metal ithanda ukuqhekeka

Isinyithi se-weld se-ER630 si-martensitic ngokupheleleyo kwaye asinayo i-delta ferrite, ngokuchaseneyo nesithambisi se-austenitic ngasinye esiqeqeshwe kuso, apho i-ferrite egciniweyo ithintela ukuqhekeka kokuqina.

Isiphumo kukuba amalungu aqhekeka kakhulu kwaye atyebile. Yinciphise ngoyilo olungcono lwamalungu, ulandelelwano lwe-weld olulinganiselayo, ufudumale kusengaphambili kwiindawo ezityebileyo, kwaye unyange ubushushu ngokukhawuleza.

Ifakwe kwiMeko A, Hayi kwi-H900

Imeko A yimeko exutywe nesisombululo, malunga ne-33 HRC, kwaye yiyo ekufuneka idityaniswe kuyo. Ithambile, ayiguquguquki kwaye iyanyamezela ukujikeleza kobushushu okufakwa yi-weld kuyo.

Ukuwelda inxalenye ye-H900 ngumsebenzi owahlukileyo. I-arc ithatha ibhendi yesinyithi esiqinileyo ngaphezu kobushushu bokuguqulwa kwaye iyibuyisele njenge-martensite engagutyungelwanga. Le nxalenye isenesatifikethi se-H900 kwaye ayisasebenzi njengayo.

Ukuba indibano kufuneka idityaniswe emva kokuba igugile, indlela ethembekileyo kukulungisa isisombululo nokulungisa yonke indawo. Ukulungisa indawo akuyonto yokulungisa, sisiphene sesibini.

Umgaqo wokulandelelanisa ogcina uninzi lweenkunkuma: weld kuqala, ubushushu buthathe okwesibini, umatshini wesithathu. Isikhokelo sonyango lobushushu lwe-17-4 PH sigubungela ileli epheleleyo.

Unyango lobushushu emva kokuWelda kwi-17-4 PH Welding: Iindlela ezintathu

Unyango lobushushu emva kokuWelda kwi-17-4 PH Welding: Iindlela ezintathu
Unyango lobushushu emva kokuWelda kwi-17-4 PH Welding: Iindlela ezintathu

Unyango lobushushu emva kokuwelda lwe-17-4 PH alulonyango olunye. Lukhetho phakathi kwezintathu, kwaye zivelisa amalungu amathathu ahlukeneyo.

Indlela 1: isisombululo se-anneal, emva koko siguge. Bamba kwi-1,038 ukuya kwi-1,040 °C, uphole, uze uguge kubushushu bemeko. Oku kubuyisela iipropati zesiseko sesinyithi kwisinyithi se-weld, i-HAZ kunye nomzali, kwaye yiloo nto ifunyanwa zii-weldments ezibalulekileyo. Iindleko ziyinyani: ukuguguleka, isikali, umthamo wesithando, kunye nokugqitywa kokugqiba emva koko.

Indlela yesi-2: ubudala kuphela, akukho sisombululo sitsha. Isinyithi esitshixiweyo kunye neHAZ zigugile endaweni yazo, masithi, kuma-482 okanye kuma-621 °C. Uninzi lokulungiswa kwentsimi lwenza oku. Iqela likaKarim litshixile ipompu eRotterdam laza layilungisa kwindawo yayo endaweni yokutsala indibano ngaphandle komgca. Yasebenza, kodwa iHAZ ayizange ibuyele kwimeko yayo epheleleyo, ngoko ke ijoyinti yayingaphantsi kweempawu zesiseko sesinyithi ukususela ngomhla wokuqala. Oko kuyamkeleka apho ijoyinti ingaxakekanga kukudinwa okanye ingavezwanga yichloride.

Indlela yesi-3: akukho PWHT. Isemthethweni kuphela nge-austenitic filler, kwinkonzo engagxininisi kakhulu, engeyiyo i-chloride.

Umzila Oko ikubuyiselayo Isiphumo esiqhelekileyo esidibeneyo Uyisebenzisa nini Umngcipheko oyintloko
Isisombululo se-anneal + ubudala Iipropati zesinyithi esisisiseko kuzo zontathu iindawo Kufuphi nentsimbi engumzali Uxinzelelo, ukudinwa kunye nenkonzo yekloridi Ukuguqulwa kunye nobukhulu; ukwenziwa kwemishini emva koko
Iminyaka kuphela Amandla esinyithi e-Weld; i-HAZ tempering engaphelelanga Umzali ongaphantsi kwi-HAZ Ukulungiswa kwentsimi, amalunga angengomsebenzi ubalulekileyo Ubunzima be-HAZ buhlala buphezulu
nanye Akukho nto kwi-HAZ Amandla amiselwe yi-filler yodwa I-Austenitic filler, inkonzo eyomileyo engadingi ngxaki I-martensite engalawulekiyo ishiywe endaweni yayo

Inkonzo emuncu iyayiqinisa ngakumbi le nto. I-NACE MR0175 / ISO 15156 ivala ubulukhuni kwi-33 HRC, nto leyo ethintela i-H900 kwaye idla ngokunyanzela iRoute 2 egugileyo okanye iRoute 1 epheleleyo. Isikhokelo seempawu ze-17-4 PH ngokwemeko sinika amanani.

Ukuba ulinganisa ixesha lesithando xa uthelekisa neempawu zamalungu, iqela lethu lokucubungula ngokwezifiso lingacaphula unyango oluhambisana nalo mbandela.

I-HAZ yindawo apho i-Joint ihluleka khona

Indawo echaphazeleka bubushushu yibhendi yesinyithi esisisiseko esishushu ngokwaneleyo ukuba siguquke kodwa singanyibiliki. Xa sipholile, siba yi-martensite engagugiyo. Sinzima kunesinyithi esitshisiweyo kunye nesinyithi esiphambili, kwaye akukho nto ngaphandle kwe-re-solution anneal iyasisusa.

Kwinkonzo ye-chloride, indawo echaphazeleka bubushushu eyi-17-4 PH yindawo yokuqalisa ukuqhekeka koxinzelelo lokubola, kuba idibanisa ubunzima obuphezulu kunye noxinzelelo oluseleyo oluphezulu. Phantsi komthwalo ojikelezayo yindawo yokuqalisa ukudinwa ngesizathu esifanayo. Inqaku lokumelana nokubola kwe-17-4 PH ligubungela indlela ye-SCC.

Ubunzima kwi-Fusion Line

Iincopho zobunzima be-weld ze-17-4 PH ngaphandle nje komgca wokudibanisa, kungekhona kwidiphozithi. Uphando lobunzima oluvavanya kuphela isinyithi se-weld luya kuphoswa kukufunda okuphezulu kwindibano, kwaye yiloo nto i-NACE eyikhathaleleyo.

Unyango lokuguga kuphela luyayinciphisa kancinci i-spike. Ukulungiswa ngokutsha kuphela kuyayisusa, yiyo loo nto uphando luyindlela ofumanisa ngayo into oyilungisileyo.

Ubushushu, i-Interpass kunye ne-Heat Input

Ibango lika-pillar lokuba i-17-4 PH welding ayifuni kufudunyezwa kwangaphambili lichanekile kwiindawo ezincinci. Iifom zeMartensite xa kuphola umoya kwaye imeko A inzima, ngoko akukho sizathu sokutshintsha ukufudumeza kwangaphambili ngendlela i-410 okanye i-420 eyidinga ngayo.

Ngaphezulu kwama-25 mm, okanye naphi na apho kuthintelwa khona kakhulu, indlela yokusebenza iyatshintsha. Ubushushu obumalunga nama-95 ukuya kwi-150 °C buqhelekile, kulawulo lwe-hydrogen kunye nokumelana nokuqhekeka endaweni yokulawula utshintsho. Yindlela yokulinganisa ukwenziwa, ayiyomfuneko ye-metallurgical yomgangatho.

Gcina ubushushu be-17-4 PH bungaphantsi kwe-150 °C. I-interpass ephezulu iyayiqinisa i-HAZ kwaye yandisa indawo ethambileyo ngaphandle kokuthenga nantoni na.

Ukufakwa kobushushu kuphakathi kwaye akubalulekile kangako kunakwi-duplex. Akukho balance ye-ferrite yokukhusela, ngoko ke ifestile ibanzi; imida bubunzima be-HAZ kunye nokugqwetheka. Uqeqesho oluphantsi lwe-hydrogen lusasebenza: izinto ezisetyenziswayo ezomileyo, ubuso obucocekileyo bamalungu, akukho kufuma.

I-Arc Blow: Ingxaki Abawelda Be-Austenitic Abangayibonayo

I-17-4 PH inamandla e-ferromagnetic kuyo yonke imeko. Abawelda be-Austenitic abacingi ngayo, kuba i-304 kunye ne-316 azinamandla e-magnetic. Kule nqanaba, i-arc ijika iye emhlabeni okanye iye kwintsimbi ekufutshane.

UDmitri uchithe iintsuku ezimbini kwi-spool ye-17-4 PH esukela into awayeqinisekile ukuba yingxaki yokugubungela igesi. I-porosity yayikwicala elinye kuphela. Isizathu yayikukubamba komhlaba ekupheleni kwe-spool yeemitha ezintandathu, itsala i-arc ngaphandle komgca.

Ukulungiswa kwezinto akuthandeki: sondeza umhlaba, wahlule ube ngamanqaku amabini, nciphisa i-arc, nciphisa umbane, okanye utshintshele kwi-AC apho inkqubo ivumela khona. Iindawo ezisandula kuhlolwa iinxalenye zemagnethi zineemagnethi kwaye nazo ziya kwenza njalo, ngoko ke qala ngokunciphisa imagnethi.

Ipropati efanayo iluncedo ekuhlolweni: ukuhlolwa kwamasuntswana emagnethi kusebenza kwi-weld egqityiweyo ye-17-4 PH, engenakunikezelwa yi-austenitic joint. Inqaku lemagnethi le-is 17-4 PH ligubungela ipropati ngokwayo.

Ukuwelda kunye nokuGqola kwe-17-4 PH: Ukuqhola kunye nokuPasa

Ukuwelda kunye nokuGqola kwe-17-4 PH: Ukuqhola kunye nokuPasa
Ukuwelda kunye nokuGqola kwe-17-4 PH: Ukuqhola kunye nokuPasa

I-welded 17-4 PH assembly idla ngokubola kwi-weld kuqala, kwaye yi-heat tint yiyo loo nto. I-heat tint ayisiyo ibala. Yi-oxide ephelelwe yi-chromium eyenzeka xa umphezulu ushushu ngokwaneleyo ukuba udibanise i-chromium kwaye ungayibuyisi.

Ukuyithambisa phezu kobushushu kubi kunokwenza nto. Ukuyithambisa kususa i-iron ekhululekileyo kwaye akunakubuyisela i-chromium esele ibotshelelwe kwi-oxide. I-weld enemibala engafakwanga yi-chromium-depleted layer evalelwe phantsi kwefilimu encinci engafakwanga, kwaye iyaphuma.

Ulandelelwano luqala nge-pickle, emva koko luphume. Ukukhupha nge-ASTM A380 kususa umaleko onombala kwaye kuveze isinyithi esitsha. Ukukhupha nge-ASTM A967 okanye i-AMS 2700 kubuyisela ifilimu ephumeyo.

Akukho siphelo silungisa iprofayili embi. Ukunqunyulwa kwe-weld kunye nokudlula kweengcambu ezingadibaniyo ziimfanta zejometri, kwaye isisombululo bubuchule, kungekhona ikhemistri.

Amaqela angafaniyo, iziqinisekiso kunye nokuhlolwa

Inkqubo yokuwelda ye-17-4 PH yi-WPS ene-PQR exhasayo, efanelekile phantsi kwe-ASME BPVC Section IX yomsebenzi woxinzelelo okanye i-AWS D17.1 yendiza. Unyango lobushushu emva kokuwelda lutshintsho olubalulekileyo, ngoko ke ukutshintsha indlela kuyayingasebenzi.

I-AWS D1.6 yikhowudi yesakhiwo esingenasici, kwaye ayibonisi i-17-4 PH njengesinyithi esisisiseko esifanelekileyo. Yiphathe loo nto njengokufuna imvume yonjineli ngaphambi kokuba ucaphule ukuhambelana kwe-D1.6.

Kwinkonzo emuncu, itshekhi ebalulekileyo luphando lobunzima kulo lonke i-HAZ, hayi uvavanyo lokutsalwa. Kuzo zonke ezinye izinto, jonga umphezulu kunye ne-radiography okanye i-ultrasound ukuze udibanise.

Inqaku lethu lezicelo ze-17-4 PH ligubungela apho la majoyinti aphela esebenza khona.

Imibuzo ebuzwa qho

Ngaba ungayishida intsimbi engagqwaliyo ye-17-4 PH?
Ewe. Ihlanganiswa rhoqo yi-GTAW, GMAW, SMAW kunye ne-SAW. Sebenzisa i-ER630 apho amandla abalulekileyo, kwaye ucwangcise unyango lobushushu emva kokudityaniswa kwesinyithi kuqala.

Yeyiphi intsimbi yokuzalisa oyisebenzisayo kwi-17-4 PH?
I-ER630 wire engenanto okanye i-electrode egqunywe yi-E630, zombini zihambelana ne-UNS S17400. I-Austenitic ER308L okanye i-ER309L isetyenziswa apho amandla adibeneyo engadingekiyo.

Ngaba i-17-4 PH ifuna ukufudunyezwa kwangaphambili?
Akukho kwiindawo ezincinci. Ngaphezulu kwama-25 mm, okanye kwindawo exineneyo, ubushushu bangaphambi kokuba bube malunga nama-95 ukuya kwi-150 °C buqhelekile kulawulo lwe-hydrogen kunye nokuqhekeka.

Ngaba i-17-4 PH ifuna unyango lobushushu emva kokuwelda?
Ukuba uneempawu ezipheleleyo zokudibanisa, ewe. Isisombululo esifakwe kwi-1,038 ukuya kwi-1,040 °C silandelwa kukwaluphala sibuyisela iimpawu zesiseko sesinyithi. Ukuguga kuphela kushiya i-HAZ ngaphantsi kwesinyithi esingumzali.

Ngaba ungayishisela i-17-4 PH kwimeko ye-H900?
Ungakwenza, kodwa akufanele. I-arc ibuyisela ibhendi yesinyithi esiqinileyo kwi-martensite engagutyungelwanga, kwaye i-assembly ayisafani nesatifikethi sayo.

Kutheni i-17-4 PH iqhekeka?
Isinyithi se-weld se-ER630 sinamandla ngokupheleleyo e-martensitic kwaye asinayo i-delta ferrite, ngoko ke sinoqhekeko xa sibambekile kakhulu. I-HAZ engaguqukiyo yenye indawo yokuqala.

Ingakanani iqondo lobushushu eliphezulu eliphakathi kwe-interpass?
Malunga ne-150 °C. I-interpass ephezulu iyayiqinisa i-HAZ kwaye yandisa indawo ethambileyo ngaphandle kokuphucula nantoni na.

Ngaba ungayishisela i-17-4 PH kwintsimbi yekhabhoni?
Ewe. I-ER309L okanye isizalisi se-nickel-base seklasi ye-ERNiCr-3, kunye nobushushu bangaphambi kunye ne-interpass elandela icala lentsimbi yekhabhoni.

Uyisusa njani i-heat tint kwi-weld ye-17-4 PH?
I-Pickle ngokwe-ASTM A380, uze u-passivate ngokwe-ASTM A967 okanye kwi-AMS 2700. I-Passivate ngaphandle kwe-pickling ivala umaleko ophelelwe yi-chromium endaweni yawo.

Ingaba i-17-4 PH isenamandla ombane emva kokuwelda?
Ewe. Uhlobo lusebenza nge-ferromagnetic kuzo zonke iimeko, kwaye ukuwelda akutshintshi loo nto. Yiyo loo nto kwenzeka i-arc blow kwaye yiyo loo nto i-MPI isebenza.

Isiphelo: Oko Kufunekayo Ngokwenene kwi-17-4 PH Welding

Ukuwelda kwe-17-4 PH kulandelana kwezigqibo ezine. Imeko igqiba indawo oza kuqala kuyo, ngoko ke iwelda kwiMeko A. Isizalisi sigqiba isinyithi esiweldayo, ngoko ke sebenzisa i-ER630 ngaphandle kokuba utshintshiselana ngabom ngamandla ngexesha lesitofu.

Emva koko unyango lobushushu lugqiba ngejoyinti, kwaye isisombululo kuphela se-anneal kunye nobudala sibuyisela iipropati zesiseko sentsimbi kuzo zontathu iindawo. Ukugqitywa kugqiba ukuba iyabola na, ngoko ke i-pickle ngaphambi kokuba uphumle.

“Sebenzisa i-ER630 kunye ne-heat treat” ayisiyonkqubo. Ngumgca wokuqala wento enye. Okunye yimeko, uthintelo, i-HAZ, uphando kunye nokugqitywa.

Ukuba ufuna i-17-4 PH yokudibanisa okutshixiweyo, yi-ode kwimeko efunwa yinkqubo kwaye ucele isatifikethi esingqina oko. Cela ikowuteshini enemeko, ifomu yemveliso kunye neenkcukacha ezidibeneyo, kwaye siya kuqinisekisa ukuba yintoni esinokuyibonelela kunye nendlela yonyango efanele ibe yiyo.